LORD 7545
Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other
Main features
- 1:1 mix ratio, 100% solids urethane adhesive
- 1.5 to 65 minute selectable working time
- Non-sag structural bonding with environmental and solvent resistance.
Product Description
LORD® 7545 is an equal-mix, two-component urethane adhesive designed for structural bonding of FRP, SMC, plastics, primed metals, and mixed-material assemblies. It combines a 1:1 mix ratio by volume, 100% solids, and a selectable working time from 1.5 to 65 minutes, depending on curative, while curing to full strength in 24 hours at 75°F (24°C). Its non-sag paste rheology, structural bond profile, and cured resistance to weathering, humidity, salt spray, and many solvents make it suitable for assemblies exposed to mixed-substrate interfaces, vertical joints, and environmental service conditions.
Product Key Features
- Equal-Mix Processing - uses a 1:1 resin-to-curative mix ratio by volume across the series to simplify dispensing setup.
- Selectable Open Time - curative options span 1.5 to 65 minutes to match line speed, part size, and assembly complexity.
- Non-Sag Rheology - remains in place on vertical or overhead surfaces to support bead control during assembly.
- Structural Bond Profile - delivers Shore D 67 hardness, 3000 psi tensile strength at break, and 72% elongation.
- Environmental Resistance - cured adhesive resists weathering, humidity, salt spray, and many solvents.
Applications
This adhesive fits composite and mixed-material assemblies that require structural bonding, controlled bead placement, and curative options matched to production timing.
- Composite Panel Bonding: Bonds FRP, SMC, and other plastics with little surface preparation and supports irregular mating surfaces.
- Plastic-to-Metal Assemblies: Bonds primed metals and dissimilar substrates where non-sag application and clamp-to-handling strength control matter.
- Exterior and Industrial Assemblies: Supports bonded joints exposed to weathering, humidity, salt spray, and downstream cleaning or painting operations.
Packaging
TDS, SDS & Technical Documents
- Technical-Datasheet-LORD-7545
- Safety-Data-Sheet-LORD-7545D
- Safety-Data-Sheet-LORD-7545A
- Tech-Tip-LORD-7545-Series-Urethane-Adhesive-Handling-Application-Notes
- Safety-Data-Sheet-LORD-7545F
- Safety-Data-Sheet-LORD-7545E
- Safety-Data-Sheet-LORD-7545D-Black
- Safety-Data-Sheet-LORD-7545G
- Safety-Data-Sheet-LORD-7545B-Black
- Safety-Data-Sheet-LORD-7545C
- Application-Guide-Structural-Adhesive-Bonding
- Safety-Data-Sheet-LORD-7545B
Technical Specifications
General Properties
Physical Properties
Thermal Properties
Mechanical Properties
Chemical Properties
Additional Information
LORD® 7545
LORD® 7545 is an equal-mix, two-component urethane adhesive system for structural bonding of FRP, SMC, plastics, primed metals, and dissimilar substrates. It uses a 1:1 mix ratio by volume, offers curative options from 1.5 to 65 minutes working time, and reaches full strength in 24 hours at 75°F (24°C). Its non-sag bead profile and cured resistance to weathering, humidity, salt spray, and many solvents support bonded assemblies exposed to mixed-material interfaces, vertical joints, and service stress.
Typical values only. Working time and handling strength depend on the selected curative.
Key Features
- 1:1 mix ratio by volume across the series to help simplify meter, mix, and cartridge setup.
- Working-time options from 1.5 to 65 minutes to help align adhesive selection with assembly takt time.
- Non-sag paste rheology to help maintain bead placement on vertical and overhead joints.
- 100% solids mixed system to help maintain bondline fill without solvent loss during cure.
- Cured resistance to weathering, humidity, salt spray, solvents, and most paint-shop cleaning steps.
Processing Summary
Process Notes
- Use within the 6-month shelf life.
- Store unopened material at or below 25°C.
- Use FIFO to maintain inventory turnover.
- No pre-treatment or degas is required.
- Remove grease, dirt, loose debris, and processing fluids.
- For plastics, use a dry rag wipe or solvent-dampened rag.
- For metals, prime or grit blast, then solvent wash for optimum bond performance.
- Plasma treatment can help on hard-to-bond materials in special cases.
- Use PTFE-lined hoses, 300 series stainless wetted metal parts, and PTFE-based seals.
- Use a compatible flouroelastomer stator for progressive cavity equipment.
- Use at least 20 static mixer elements for 50 mL cartridges and 24 elements for 200 mL or MMD dispense.
- Do not manually agitate before transfer. Manual mixing can entrain air and disturb mix ratio.
- Dispense within working time. Discard material once working time is exceeded.
- Perform ratio checks at least once per day or at the start of each shift. Flag deviations greater than ±5%.
- Level cartridge plungers before attaching the mixer tip.
- When switching within the same base chemistry, purge 3 times the MMD line volume. For different base chemistries, perform a full wetted-parts teardown.
Engineering Data for LORD® 7545
Resin Properties, 7545-A Resin
| Property | 7545-A Resin | Condition / method |
|---|---|---|
| Appearance | Brown paste | Per technical data sheet |
| Viscosity | 25,000 to 70,000 cP | Brookfield, @ 77°F (25°C) |
| Density | 12.5 to 12.8 lb/gal (1498 to 1534 kg/m³) | Per technical data sheet |
| Flash point | >200°F (>93°C) | Closed cup |
Curative Properties at 77°F (25°C)
| Property | 7545-G Curative | 7545-B Curative | 7545-C Curative | 7545-D Curative | 7545-E Curative | 7545-F Curative |
|---|---|---|---|---|---|---|
| Appearance | Black paste | Off-white or black paste | Off-white paste | Off-white or black paste | Off-white paste | Off-white paste |
| Viscosity | 230,000 to 650,000 cP | 230,000 to 650,000 cP | 230,000 to 650,000 cP | 230,000 to 650,000 cP | 230,000 to 650,000 cP | 230,000 to 650,000 cP |
| Density | 10.8 to 11.2 lb/gal (1294 to 1342 kg/m³) | 10.8 to 11.2 lb/gal (1294 to 1342 kg/m³) | 10.8 to 11.2 lb/gal (1294 to 1342 kg/m³) | 10.6 to 11.0 lb/gal (1270 to 1318 kg/m³) | 10.6 to 11.0 lb/gal (1270 to 1318 kg/m³) | 10.5 to 11.1 lb/gal (1258 to 1330 kg/m³) |
| Flash point | >200°F (>93°C) | >200°F (>93°C) | >200°F (>93°C) | >200°F (>93°C) | >200°F (>93°C) | >200°F (>93°C) |
Mixed Resin and Curative Processing Windows, @ 75°F (24°C)
| System | Mix ratio by volume | Mix ratio by weight | Solids content by weight | Working time | Time to handling strength |
|---|---|---|---|---|---|
| 7545-A/G | 1:1 | 1:0.87 | 100% | 1.5 min | 10 min |
| 7545-A/B | 1:1 | 1:0.87 | 100% | 3 to 5 min | 30 min |
| 7545-A/C | 1:1 | 1:0.87 | 100% | 6 to 8 min | 60 min |
| 7545-A/D | 1:1 | 1:0.85 | 100% | 11 to 18 min | 90 min |
| 7545-A/E | 1:1 | 1:0.85 | 100% | 22 to 38 min | 2 to 3 hr |
| 7545-A/F | 1:1 | 1:0.85 | 100% | 45 to 65 min | 4 to 5 hr |
Cured Properties
Cure basis: full strength in 24 hours at 75°F (24°C), depending on curative used.
| Property | Typical value | Test method |
|---|---|---|
| Hardness | Shore D 67 | Per technical data sheet |
| Tensile strength at break | 3000 psi (20.7 MPa) | ASTM D882 |
| Elongation | 72% | ASTM D882 |
| Young’s modulus | 22,200 psi (153 MPa) | ASTM D882 |
| Glass transition temperature (Tg) | 116°F (47°C) | ASTM D3418 |
| Moisture absorption | <1% | ASTM D570 |
Bond Performance
| Condition | CFRP | ABS | PC/ABS | E-coated steel |
|---|---|---|---|---|
| Lap shear @ 70°F (21°C), psi (MPa) / failure mode | 2900 (20.0) / SF | 550 (3.8) / SF | 900 (6.2) / SF | 2350 (16.2) / COH |
| Lap shear @ -40°F (-40°C), psi (MPa) / failure mode | 2600 (17.9) / SF | 400 (2.8) / SF | 550 (3.8) / SF | 3300 (22.7) / ADH |
| Lap shear @ 150°F (65°C), psi (MPa) / failure mode | 1150 (7.9) / COH | 350 (2.4) / COH | 550 (3.8) / COH | 1100 (7.6) / COH |
| Lap shear after 500 hr @ 150°F (65°C), 85% RH, psi (MPa) / failure mode | 2700 (18.6) / SF | 550 (3.8) / SF | 750 (5.2) / COH | 2400 (16.5) / COH |
| Lap shear after 168 hr water immersion @ 150°F (65°C), psi (MPa) / failure mode | 2650 (18.3) / COH/SF | 550 (3.8) / SF | 650 (4.5) / COH/SF | 2450 (16.9) / COH |
| Lap shear after 500 hr salt spray exposure, psi (MPa) / failure mode | 2650 (18.3) / SF | 550 (3.8) / SF | 650 (4.5) / SF | 2400 (16.5) / COH |
| Lap shear after 500 hr @ 150°F (65°C), psi (MPa) / failure mode | 2900 (20.0) / SF | 550 (3.8) / SF | 850 (5.8) / SF | 1500 (10.3) / COH |
| T-peel, pli (N/mm) / failure mode | - | - | - | 33 (5.8) / COH |
Where LORD® 7545 Fits
- Bonds FRP, SMC, other plastics, and primed metals.
- Non-sag paste supports vertical and overhead bond lines.
- Cured system resists weathering, humidity, and salt spray.
- 1:1 mix ratio by volume across all curative options.
- Working time can be selected from 1.5 to 65 minutes.
- Large gaps may be filled where surfaces are irregular.
- Off-white cured adhesive supports acceptable visible appearance.
- Painting and most cleaning processes do not affect bond strength.
- Solvent resistance after cure supports downstream finishing steps.
See LORD® 7545 in Use
Practical view of cartridge dispensing, bead placement, part mating, and assembly handling for LORD® 7545. A quick visual reference when selecting working time, reviewing clamp-to-handling timing, or aligning dispense practice with the 1:1 resin and curative system setup.
Standard Packaging & Technical Help
- 50 mL cartridges
- 200 mL cartridges
- 5 gallon pails
- 55 gallon drums
- Match curative selection to working time, handling strength, and part size.
- Review equipment compatibility for PTFE, stainless, seals, and stator materials.
- Confirm surface prep, static mixer length, and ratio-check method for your line.
- Support purge strategy and changeover planning for cartridge or MMD dispense.
Tips and Troubleshooting
| Issue | Recommended Action |
|---|---|
| Poor wetting or lower bond strength |
|
| Incomplete cure or off-ratio mix |
|
| Equipment compatibility or changeover risk |
|